Plan
Comptes Rendus

Tin ions in float glass cause anomalies
Comptes Rendus. Chimie, Volume 5 (2002) no. 11, pp. 759-763.

Résumés

There are two anomalies at the tin bath side of silicate float glasses caused by the in-diffusion of tin into the glass melt, the tin hump in the micrometer region and the phenomenon of bloom, a microscopic wrinkling at the glass surface after reheating in air. A diffusion–reaction model is developed to explain the tin hump and it is shown that it occurs only for Fe2O3-rich (> 0.5 wt%) silicate float glasses. The bloom effect, on the other hand, is found only for Fe2O3-poor (< 0.13 wt%) silicate float glasses. It could be demonstrated that these float glasses have a high tin peak already near the surface (< 100 nm) and that after annealing its height is strongly increased. The drastically altered surface properties lead to a buckling at the surface.

À la surface de verres flottés, trempés dans un bain d’étain, deux anomalies apparaissent, provoquées par la diffusion d’étain dans le verre fondu : une bosse d’étain, de l’ordre du micromètre, et le phénomène de fleurage, ride microscopique sur la surface du verre, observé après réchauffage dans l’air. Un modèle de diffusion réactive est développé pour expliquer la bosse d’étain. Il est démontré que ce phénomène apparaît seulement pour des verres flottés au silicate, riches en Fe2O3 (> 0,5% en masse). L’effet de fleurage n’est observé que pour des verres flottés au silicate, pauvres en Fe2O3 (< 0,13% en masse). On pourrait démontrer que ces verres flottés présentent déjà un pic élevé d’étain près de la surface (< 100 nm) et que la hauteur de ce pic augmente considérablement après le recuit. Les changements drastiques des propriétés de surface provoquent des boursouflures à la surface.

Métadonnées
Reçu le :
Accepté le :
Publié le :
DOI : 10.1016/S1631-0748(02)01436-4
Keywords: float glass, tin diffusion, tin hump, bloom, tin anomalies
Mots-clés : verres flottés, diffusion d’étain, bosse d’étain, fleurage, anomalies d’étain

Günther Heinz Frischat 1

1 Institut für Nichtmetallische Werkstoffe, Technische Universität Clausthal, Zehntnerstraße 2A, 38678 Clausthal-Zellerfeld, Germany
@article{CRCHIM_2002__5_11_759_0,
     author = {G\"unther Heinz Frischat},
     title = {Tin ions in float glass cause anomalies},
     journal = {Comptes Rendus. Chimie},
     pages = {759--763},
     publisher = {Elsevier},
     volume = {5},
     number = {11},
     year = {2002},
     doi = {10.1016/S1631-0748(02)01436-4},
     language = {en},
}
TY  - JOUR
AU  - Günther Heinz Frischat
TI  - Tin ions in float glass cause anomalies
JO  - Comptes Rendus. Chimie
PY  - 2002
SP  - 759
EP  - 763
VL  - 5
IS  - 11
PB  - Elsevier
DO  - 10.1016/S1631-0748(02)01436-4
LA  - en
ID  - CRCHIM_2002__5_11_759_0
ER  - 
%0 Journal Article
%A Günther Heinz Frischat
%T Tin ions in float glass cause anomalies
%J Comptes Rendus. Chimie
%D 2002
%P 759-763
%V 5
%N 11
%I Elsevier
%R 10.1016/S1631-0748(02)01436-4
%G en
%F CRCHIM_2002__5_11_759_0
Günther Heinz Frischat. Tin ions in float glass cause anomalies. Comptes Rendus. Chimie, Volume 5 (2002) no. 11, pp. 759-763. doi : 10.1016/S1631-0748(02)01436-4. https://comptes-rendus.academie-sciences.fr/chimie/articles/10.1016/S1631-0748(02)01436-4/

Version originale du texte intégral

Le texte intégral ci-dessous peut contenir quelques erreurs de conversion par rapport à la version officielle de l'article publié.

1 Introduction

Float glasses are produced worldwide in huge amounts and are among the most important technical glasses. It has long been known that tin ions can penetrate into the bath side of the float glass melt during the production process 〚1–3〛. Consequently, float glasses have two quite dissimilar sides. At the tin bath side, the performance of the glass surface is mainly determined by the in-diffused tin. At the atmosphere side, on the other hand, the surface is melt-formed (fire-polished) and displays pristine nature. Of course, both sides can be altered during further handling and/or storage.

There are especially two anomalies at the tin bath side of silicate float glasses that puzzle glass technologists since long, viz:

  • • the so-called tin hump or bump, a peak in tin concentration in the micrometer region of several glasses 〚3–6〛,
  • • the phenomenon of bloom, a greyish haze on other glasses after reheating in air, caused by a microscopic wrinkling at the surfaces 〚1, 7, 8〛.

Despite the many experimental and theoretical efforts to understand these interaction processes between tin and the glass melt in the float chamber, these are still largely unclear. Therefore, we initiated a joint-laboratory study on ‘tin in float glass’. Its aim was to measure precisely the in-depth profiles of all relevant species in the nanometer and the micrometer regions of the glasses, the in-depth profile of the Sn2+/Sn4+ ratio, and also the topographies of as-received and fractured glass surfaces on a nanometer scale. Based on the results, models were developed to explain the two mentioned anomalies.

2 Some experimental findings

Eight commercial float glasses with a thickness of 4 mm were investigated. Six of them were soda-lime silicate float glasses with Fe2O3 contents ranging from 0.017 to 1.80 wt%, and the two others were floated borosilicate glasses having Fe2O3 contents of ∼0.02 wt%, respectively 〚9〛. With the application of electron probe microanalysis (EPMA), Rutherford backscattering spectrometry (RBS) and Secondary Neutral Mass Spectrometry (SNMS), the complete in-depth profiles of all relevant elements from the first few nanometers to several micrometers could be obtained 〚10, 11〛. Conversion electron Mössbauer spectrometry (CEMS) was used to describe the Sn2+/Sn4+ ratio as a function of penetration depth 〚12, 13〛, and high-resolution atomic force microscopy (AFM) was applied to study the topographies of the different glass surfaces 〚14, 15〛.

3 Tin hump in the micrometer region

Fig. 1 displays the tin concentration profiles in a silicate float glass with an overall Fe2O3 content of 0.605 wt% and a Fe2+/(Fe2+ + Fe3+) ratio of 23.9. Irrespective of the method, a satellite peak in the tin profile between about 6 and 8 μm can be seen for the 4-mm float glasses. Similar peaks are found in other Fe2O3-rich float glasses, showing surface tin concentrations between 0.25 and 0.35 wt%. The borofloat glasses and the silicate float glasses with a low overall Fe2O3 content (< 0.2 wt%) did not show a tin hump within the present experimental error. A silicate float glass with 0.56 wt% Fe2O3, which had been prepared under reducing conditions (Fe2+/〚Fe2+ + Fe4+〛 = 60), did equally not show a tin hump.

Fig. 1

RBS, SNMS, EPMA and CEMS tin depth profiles in a float glass with 0.605 wt% Fe2O3 (the SNMS profile was shifted by –0.3 at%).

How can this anomalous peak be explained? The following conditions are assumed valid:

  • • when the glass melt, which has been prepared under oxidizing conditions, enters the float chamber, a very strong and rapid change occurs in its oxidation state near the surface; this causes the redox processes

    2Fe3++3O2-+Sn02Fe2++2O2-+SnObathside
    (see also the schematic in Fig. 2);

  • • the Fe2+ ions (possibly also ions like Na+ or Ca2+) enable an ongoing penetration of Sn2+ ions into the glass melt by an ion-exchange process

    Sn2+Fe2+

  • • the formation of Sn4+ ions in the glass is possible only if Sn2+ and oxidation partners such as Fe3+ (possibly also S6+) are simultaneously available; according to Fig. 2, this is possible only in deeper parts of the melt; there this redox reaction proceeds according to

    Sn2++2Fe3+Sn4++2Fe2+
    (since the Sn4+ ions act as network formers 〚16〛, they become highly immobile in the glass network);

  • • as a consequence, the convolution of the decreasing CSn2+ profile with the increasing CFe3+ profile, divided by the decreasing CFe2+ profile, results in a peak similar to that known for the Sn4+ profiles obtained by CEMS 〚12〛 (see Fig. 3).

Fig. 2

Schematic iron profiles (bath side) at t = 0 after the glass melt has entered the float chamber.

Fig. 3

Model showing the tin hump as an interaction between diffusion and redox processes.

This diffusion-reaction model thus explains the occurrence of the tin hump in Fe2O3-rich float glasses under the assumption that the oxidation state of the glass surface changes drastically and rapidly when it enters the strongly reducing float chamber. Everything else follows as a consequence.

4 The phenomenon of bloom

It is generally accepted that the phenomenon of bloom is related to the oxidation of Sn2+ to Sn4+ during reheating of those float glasses in air, whose ‘tin count’ (determined by X-ray fluorescence spectrometry) shows a distinct value 〚1, 8〛. The Sn4+ acts as a network former in the glass structure 〚16〛, changing the glass properties in a superficial layer.

Fig. 4 shows an AFM image of a standard float glass with bloom. This glass has an overall Fe2O3 content of 0.13 wt% and had been annealed as a 100 mm × 100 mm sheet for 1 h at 670 °C, followed by a cooling with the natural furnace rate. The wave pattern produced at the surface is irregular, has a wavelength of ∼3 μm and shows an rms roughness of 65 to 75 nm. The occurrence of bloom is somewhat dependent on sample size, geometry, and the heating program. Annealing in reducing atmosphere does not produce bloom and borofloat glasses do not show this effect under any condition 〚15〛. However, within this work, bloom could be evidenced only on the surfaces of white soda-lime silicate float glasses with a low Fe2O3 content (≤ 0.13 wt%), whereas green and blue glasses with higher Fe2O3 contents (> 0.5 wt%) did not develop bloom.

Fig. 4

AFM height mode image of a standard float glass surface (0.13 wt% Fe2O3) showing bloom after annealing for 1 h at 650 °C in air.

How can this Fe2O3-dependence be explained? Fig. 5 displays that the Sn in-depth profiles of the float glasses investigated in the as-received state are quite different in the first 100 nm from the surface. Whereas the silicate glasses with low Fe2O3 contents show SnO2 surface concentrations up to 7 wt% and a steep gradient in these profiles (curve 1: glass with 0.017 wt% Fe2O3), the SnO2 profiles of the borofloat and the silicate float glasses with high Fe2O3 contents have lower surface concentrations < 2.4 wt% and a much smoother decrease from the surface to the bulk (curve 2: glass with 1.80 wt% Fe2O3). After annealing these glasses for 1 h at 650 °C in air, this tendency becomes even stronger (curve 3: glass with 0.017 wt% Fe2O3). On the other hand, the mentioned annealing step smoothens the SnO2 profile of the Fe2O3-rich glasses even further (curve 4: glass with 1.80 wt% Fe2O3). Thus, one can conclude that during annealing in air a tin species is forced to diffuse from the interior to the surface in the case of the silicate float glasses with low Fe2O3 contents, whereas a diffusion process in the opposite direction obviously takes place in the case of the glasses with the high Fe2O3 contents.

Fig. 5

SNMS tin in-depth profiles of two float glasses: curve 1, Fe2O3 content 0.017 wt%, as-received; curve 2, Fe2O3 content 1.80 wt%, as-received; curve 3, Fe2O3 content 0.017 wt%, 1 h at 650 °C; curve 4, Fe2O3 content 1.80 wt%, 1 h at 650 °C.

As already mentioned, a very strong and rapid change occurs in the oxidation state of the glass melt when it enters the float chamber, see also equations (1) and (2) and Fig. 2. There are mainly the Fe2+ ions that enable the penetration of Sn2+ ions into the glass melt by an ion exchange process. Since the total number of Fe2+ ions is very low in the case of a low-Fe2O3 glass, a small part of these Sn2+ ions can diffuse into the glass only. Consequently, a steep tin (mainly Sn2+) gradient is formed near the surface. In the case of a high-Fe2O3 glass, the total number of Fe2+ ions is high. This enables a far-reaching penetration of Sn2+ ions into the glass melt. A gradient in tin concentration does not occur near the surface, however, this glass tends to form an anomalous tin (Sn4+) hump in the micrometer region 〚9〛.

When a low-Fe2O3 glass is annealed in air, most of the Sn2+ ions near the surface are oxidized to Sn4+ and depletion in Sn2+ occurs there. This now causes an opposite gradient in the Sn2+ concentration with the consequence of a reversed Sn2+ diffusion from the interior to the surface. When reaching the surface region, these Sn2+ ions are also oxidized to Sn4+, finally forming a very high and steep tin (Sn4+) peak near the very surface. Since the Sn4+ ions act as network formers in the glass structure 〚16〛, they are highly immobile. When a high-Fe2O3 glass is annealed in air, the Sn2+ ions near the surface are also oxidized to Sn4+. However, the concentration of Sn2+ ions there is low and there is no steep gradient. Moreover, since also the Sn4+ hump in the micrometer region is formed, obviously most of the Sn2+ ions are trapped there as Sn4+ and a specific tin enrichment near the surface is unlikely. A tin diffusion process from the interior to the surface was also found by 〚4, 7, 17, 18〛.

The high-tin (Sn4+) hump near the very surface of the float glasses changes their properties strongly in the region < 100 nm 〚15〛. Thus, for example, the viscosity, the glass-transition temperature, and the Young’s modulus are increased, whereas the thermal expansion coefficient is decreased. In analogy to thin film technology, a simplified model was set up and a free buckling length of ∼2.3 μm could be estimated for the wrinkling of the bloom surface 〚15〛. This value is in reasonable agreement with the experiment (Fig. 4).

5 Conclusions

Different 4 mm thick commercial float glasses were investigated. A tin hump (satellite peak) between 6 and 8 μm from the glass surface could be evidenced only for Fe2O3-rich (> 0.5 wt%) silicate float glasses. To explain this anomaly, a diffusion-reaction model was developed under the assumption that the oxidation state of the glass surface changes drastically and rapidly when the oxidized glass melt enters the strongly reducing float chamber. The phenomenon of bloom, a greyish haze causing a microscopic wrinkling of the surface, was found on silicate glasses only with a low Fe2O3 content (< 0.13 wt%) after annealing them in air. In that case, a very high and steep tin (Sn4+) peak is formed near the surface (< 100 nm), mainly because of a reversed Sn2+ diffusion process from the interior to the surface. This high Sn4+ peak near the surface changes the properties strongly, leading finally to a buckling there.

Acknowledgements

The author wishes to thank the ‘Tin in float glass’ team: Drs G. Heide, C. Müller-Fildebrandt, D. Moseler, W. Meisel (Mainz) and Prof. F. Rauch (Frankfurt/Main). He also appreciates the financial support of the AiF (Köln), HVG (Frankfurt/Main), utilizing resources of the BMWi (Bonn).


Bibliographie

[〚1〛] L.A.B. Pilkington Proc. R. Soc. Lond., A 314 (1969), p. 1

[〚2〛] R. Brückner; J.M.F. Navarro Glastech. Ber., 44 (1971), p. 361

[〚3〛] J.S. Sieger J. Non-Cryst. Solids, 19 (1975), p. 213

[〚4〛] C.G. Pantano; V. Bojan; M. Verita; F. Geotti-Bianchini; S. Hreglich 2nd ESG Conference, Venice, Italy (1993, p. 285)

[〚5〛] K.F.E. Williams; C.E. Johnson; J. Greenglass; B.P. Tilley; D. Gelder; J.A. Johnson J. Non-Cryst. Solids, 211 (1997), p. 164

[〚6〛] A. Mishra; G.A. Pecoraro; T.E. Paulson; C.G. Pantano Ceram. Trans., 82 (1998), p. 205

[〚7〛] M. Laube; F. Rauch Fresenius J. Anal. Chem., 353 (1995), p. 408

[〚8〛] K.F.E. Williams; M.F. Thomas; J. Greenglass; J.M. Bradshaw Glass Technol., 40 (1999), p. 103

[〚9〛] G. Heide; C. Müller-Fildebrandt; D. Moseler; G.H. Frischat; W. Meisel; A. Maldener; A. Zhouine-Thimm; F. Rauch Glastech. Ber. Glass Sci. Technol., 73 C 2 (2000), p. 321

[〚10〛] C. Müller-Fildebrandt PhD thesis, Technische Universität Clausthal, 2000

[〚11〛] G.H. Frischat; C. Müller-Fildebrandt; D. Moseler; G. Heide J. Non-Cryst. Solids, 283 (2001), p. 246

[〚12〛] W. Meisel Glastech. Ber. Glass Sci. Technol., 72 (1999), p. 291

[〚13〛] W. Meisel Glastech. Ber. Glass Sci. Technol., 73 C 2 (2001), p. 311

[〚14〛] D. Moseler PhD thesis, Technische Universität Clausthal, 2001

[〚15〛] D. Moseler; G. Heide; G.H. Frischat Glass Sci. Technol., 75 (2002), p. 174

[〚16〛] J.F. Bent; A.C. Hannon; D. Holland; M.M.A. Karim J. Non-Cryst. Solids, 232–234 (1998), p. 300

[〚17〛] S. Takeda; R. Akiyama; H. Hosono J. Non-Cryst. Solids, 281 (2001), p. 1

[〚18〛] Y. Hayashi; R. Akiyama; M. Kudo Surf. Interface Anal., 31 (2001), p. 87


Cité par

  • Patrice LEHUÉDÉ Lead in Glasses, Lead in Glassy Materials in Cultural Heritage (2024), p. 155 | DOI:10.1002/9781394265411.ch7
  • Mattia Biesuz; Gino Mariotto; Michele Cassetta; Ovidiu Ersen; Dris Ihiawakrim; Petr Haušild; Paolo Giopato; Alessandro Martucci; Mauro Bortolotti; Vincenzo M. Sglavo; Gian D. Sorarù Solid‐State Field‐Assisted Ion Exchange (Ag → Na) in Soda–Lime Float Glass: Tin Versus Air Side, Advanced Engineering Materials, Volume 25 (2023) no. 18 | DOI:10.1002/adem.202201572
  • Hiroyuki Inano; Yasuhiro Akemoto; Ken Asakura Upcycling of fluorescent light tube glass via kiln-casting using its properties, Glass Structures Engineering, Volume 8 (2023) no. 2, p. 303 | DOI:10.1007/s40940-022-00199-5
  • Andrew L. Ogrinc; Yuxing Zhou; Seung Ho Hahn; Yen-Ting Lin; Seong H. Kim Revealing the structure of the sodium-leached layer of soda lime silica glass: A comprehensive spectroscopic analysis, Journal of Non-Crystalline Solids, Volume 600 (2023), p. 121989 | DOI:10.1016/j.jnoncrysol.2022.121989
  • Cesar A. Nieves; Andrew L. Ogrinc; Seong H. Kim; Eugene Furman; Michael T. Lanagan Ion migration study in acid‐leached soda–lime–silica glass by thermally stimulated depolarization current analysis, Journal of the American Ceramic Society, Volume 106 (2023) no. 7, p. 4103 | DOI:10.1111/jace.19064
  • Clarissa Justino de Lima; Brandon Aldinger; Peter de Haan; Telesilla Bristogianni; Fred Veer Effects of composition on the durability and weathering of flat glass, Glass Structures Engineering, Volume 7 (2022) no. 2, p. 139 | DOI:10.1007/s40940-022-00175-z
  • Yoshitaka Saijo; Yuichi Suzuki; Ryoji Akiyama; Masahiro Shimizu; Yasuhiko Shimotsuma; Kiyotaka Miura Speciation analysis of tin at the tin side of float glass by solvent extraction combined with a stepwise etching technique, Journal of Non-Crystalline Solids, Volume 592 (2022), p. 121752 | DOI:10.1016/j.jnoncrysol.2022.121752
  • Marcos Cota‐Leal; Jorge A. García‐Valenzuela Chemical Solution Deposition of Al(OH)3‐AlOOH Films: Application for Surface Sensitizing of Rigid and Flexible Substrates to Improve the Adhesion in Coating Technology Areas, ChemistrySelect, Volume 6 (2021) no. 24, p. 6083 | DOI:10.1002/slct.202101449
  • Stephanie Reiß; Rolf Grieseler; Stefan Krischok; Edda Rädlein The influence of Sahara sand on the degradation behavior of float glass surfaces, Journal of Non-Crystalline Solids, Volume 479 (2018), p. 16 | DOI:10.1016/j.jnoncrysol.2017.09.055
  • Zheng Meng; Wang Hong; Yongbin Wang; Hong Jiang Model of diffusion of sulfur in soda-lime-silicate glass: An experimental and comparative study, Journal of Wuhan University of Technology-Mater. Sci. Ed., Volume 32 (2017) no. 1, p. 76 | DOI:10.1007/s11595-017-1561-6
  • Maximilian Heinz; Vasiliy V. Srabionyan; Aram L. Bugaev; Vasiliy V. Pryadchenko; Egor V. Ishenko; Leon A. Avakyan; Yan V. Zubavichus; Jürgen Ihlemann; Jörg Meinertz; Eckhard Pippel; Manfred Dubiel; Lusegen A. Bugaev Formation of silver nanoparticles in silicate glass using excimer laser radiation: Structural characterization by HRTEM, XRD, EXAFS and optical absorption spectra, Journal of Alloys and Compounds, Volume 681 (2016), p. 307 | DOI:10.1016/j.jallcom.2016.04.214
  • References, Glass (2014), p. 367 | DOI:10.1002/9783527679461.refs
  • Meng Zheng; Hong Wang; Tao Haizheng; Huang Yourong; Jiang Hong The effect of tin on sulfur K-edge X-ray absorption near edge structure spectra of soda–lime–silicate glass: An experimental and comparative study, Journal of Non-Crystalline Solids, Volume 383 (2014), p. 71 | DOI:10.1016/j.jnoncrysol.2013.04.027
  • Rémi Girard; Annelise Faivre; Florence Despetis; G. Pharr Crack Healing by Thermal Treatment in Float Glass: The Effect of Tin, Journal of the American Ceramic Society, Volume 97 (2014) no. 11, p. 3463 | DOI:10.1111/jace.13140
  • E. Cattaruzza; M. Mardegan; T. Pregnolato; G. Ungaretti; G. Aquilanti; A. Quaranta; G. Battaglin; E. Trave Ion exchange doping of solar cell coverglass for sunlight down-shifting, Solar Energy Materials and Solar Cells, Volume 130 (2014), p. 272 | DOI:10.1016/j.solmat.2014.07.028
  • Zheng Meng; Wang Hong; You Rong Huang; Jin Zhen Wang; Yao Hui Li; Di Shi; Hong Jiang The Oxidation State of Sulfur on the Air Side Surface of Soda-Lime Float Glass as Determined by X-Ray Absorption near Edge Structure Spectra, Materials Science Forum, Volume 743-744 (2013), p. 316 | DOI:10.4028/www.scientific.net/msf.743-744.316
  • Cornelia Bähr; Elisabeth Stammen; Sarah Zahlten; Stefan Böhm; Klaus Dilger; Jochen Büchs Refining bioreactor design using autoclavable glass bonding, Advances in Bioscience and Biotechnology, Volume 02 (2011) no. 04, p. 233 | DOI:10.4236/abb.2011.24034
  • Qin Zhang; Zejing Chen; Zhixin Li Simulation of tin penetration in the float glass process (float glass tin penetration), Applied Thermal Engineering, Volume 31 (2011) no. 6-7, p. 1272 | DOI:10.1016/j.applthermaleng.2010.12.030
  • Jiin-Jyh Shyu; Chih-Hsien Yeh Influence of heating atmosphere on the properties of stannous phosphate glass, Journal of Materials Science, Volume 46 (2011) no. 7, p. 2173 | DOI:10.1007/s10853-010-5054-7
  • A.-M. Flank; P. Lagarde; J. Jupille; H. Montigaud Redox profile of the glass surface, Journal of Non-Crystalline Solids, Volume 357 (2011) no. 16-17, p. 3200 | DOI:10.1016/j.jnoncrysol.2011.03.046
  • P Lagarde; A-M Flank; J Jupille; H Montigaud Oxidation state of sulfur, iron and tin at the surface of float glasses, Journal of Physics: Conference Series, Volume 190 (2009), p. 012079 | DOI:10.1088/1742-6596/190/1/012079
  • Hoikwan LEE; Mangyu PARK; Wonho KANG Effect of barium ions on K2O-TiO2-SiO2 glass soaked in molten Ba(NO3)2, Journal of the Ceramic Society of Japan, Volume 117 (2009) no. 1369, p. 1044 | DOI:10.2109/jcersj2.117.1044
  • E. C. Ziemath; V. D. Araújo; C. A. Escanhoela Compositional and structural changes at the anodic surface of thermally poled soda-lime float glass, Journal of Applied Physics, Volume 104 (2008) no. 5 | DOI:10.1063/1.2975996
  • References, Glass (2007), p. 353 | DOI:10.1002/9783527617029.refs
  • Harald Behrens; Miriam Haack Cation diffusion in soda-lime-silicate glass melts, Journal of Non-Crystalline Solids, Volume 353 (2007) no. 52-54, p. 4743 | DOI:10.1016/j.jnoncrysol.2007.05.178
  • B.Z. Saggioro; E.C. Ziemath Changes of physical properties of glass surfaces exposed to KNO3 vapors, Journal of Non-Crystalline Solids, Volume 352 (2006) no. 26-27, p. 2783 | DOI:10.1016/j.jnoncrysol.2006.03.052
  • U. Hoffmann; G. Heide; G.H. Frischat Reactions between sol–gel coatings and some technical glass substrates during consolidation, Journal of Non-Crystalline Solids, Volume 351 (2005) no. 43-45, p. 3562 | DOI:10.1016/j.jnoncrysol.2005.08.032

Cité par 27 documents. Sources : Crossref


Commentaires - Politique